Loading...

Wenzhou Tuopu Glasses Co.,Ltd

Metal Frame Plating: Salt Spray Hours, Coating Thickness and Nickel Release

Timeㄩ2026/11/28AuthorㄩadminFlowㄩ 10



Plating is the part of a metal frame that fails first and is specified last. Buyers routinely approve a finish from a photograph and then discover, two seasons later, that a third of the shipment has gone dull at the temple tips or that a market has rejected the goods on a nickel test that nobody ordered.

Three independent questions sit inside the word "plating": will it resist corrosion, will it stay on, and will it release nickel. They are tested differently, they fail for different reasons, and one of them is a legal gate rather than a quality preference.

Salt spray hours measure one thing

The salt spray test exposes the finished frame to a continuous fine mist of neutral salt solution under controlled conditions, and the number quoted in a specification is the hours completed before visible base-metal corrosion appears. The hours are not a quality score; they are a ranking under one specific accelerated condition.

What the hours actually tell you:

﹞      It is an accelerated corrosion test, not a wear test.A frame that survives 96 hours is not necessarily better in daily use than one that survives 48, though it is a reasonable proxy for coating integrity.

﹞      Edges and holes fail first.Coating is always thinner on a cut edge or around a drilled hole, so the failure site is predictable and should be the place the inspector looks.

﹞      The verdict needs a definition."No corrosion" is meaningless without an area threshold. Most order specifications define failure as corrosion products covering more than a stated percentage of a defined surface, excluding edges.

﹞      White and red products mean different things.On plated steel, white corrosion is the zinc or nickel layer breaking down; red corrosion means the base metal has been reached. A report that does not distinguish them cannot be compared with another report.


Duration

Where it is used

What it implies about the coating stack

24 hours

Entry-level fashion programmes, short-season SKUs

Thin nickel with a decorative chromium flash; adequate if the frame is not expected to survive daily wear for years

48 hours

Mainstream order specification for most European and North American retail

Nickel layer in the mid single digits in micrometres, full coverage on edges

72每96 hours

Premium programmes, humid markets, brands with long warranties

Thicker barrier layer, controlled bath chemistry, careful racking to avoid contact marks


The coating stack, and which layer does the work

Decorative plating on eyewear is almost always a stack rather than a single layer, and each layer has a different job. Understanding the stack explains why quoting a single thickness number is not enough.


Layer

Typical thickness

Function

Copper strike

0.5每2 µm

Adhesion to the base metal and levelling of surface defects

Nickel

3每10 µm

The corrosion barrier and the layer that carries most of the durability

Decorative chromium

0.1每0.3 µm

Hardness, wear resistance and the final colour; too thin to protect on its own

PVD coating

0.5每2 µm

Colour and wear resistance without nickel, but limited corrosion barrier

Gold flash

0.03每0.1 µm

Colour only; wears through quickly at contact points


The practical consequence is that the nickel layer, not the top coat, determines whether the frame survives. A thick decorative chromium layer over a thin nickel layer looks no different on the shelf and fails much sooner. When a supplier quotes "chrome plated", the question to ask is the nickel thickness underneath.


PVD is not automatically better.PVD gives excellent colour and wear resistance and avoids nickel entirely, which is valuable for skin-sensitive markets. But a sub-micron PVD layer over a poorly prepared substrate can corrode at pinholes faster than a well-built nickel-chromium stack. The substrate preparation matters more than the coating name.

Nickel release is a legal gate, not a preference

Under REACH Annex XVII, entry 27, articles intended to come into direct and prolonged contact with the skin must not release more than 0.5 micrograms of nickel per square centimetre per week. Spectacle frames fall squarely inside that definition: the temples rest on the skin, the front touches the nose and cheeks, and metal nose pads or their arms are in continuous contact.

Two things about this requirement catch buyers out.

﹞      The test is a release test, not a content test.A nickel-containing alloy can comply if the coating is intact and the release is low; a low-nickel alloy can fail if the surface is porous. Compliance comes from EN 1811 release testing, preceded by EN 12472 simulated wear and corrosion, which is designed to represent two years of use.

﹞      "Nickel free" is a claim, not a material description.It needs the same test evidence as a release claim, because trace nickel is present in many alloys and in plating baths. A supplier statement is not a test report.

The parts that matter are the ones people forget: hinge screws, the metal core inside an acetate temple, spring housings and any decorative rivet that sits against the skin. A titanium front with a stainless screw can still fail a market's nickel requirement if the screw is the wrong grade.

Failure modes that show up in production


Symptom

Root cause

What to change

Blistering or peeling at edges

Insufficient cleaning before plating, or coating too thin at the edge

Pre-treatment sequence and racking position

Corrosion at a single point

Pinhole in the coating, often over an inclusion in the base metal

Base metal quality and polishing before plating

Patchy colour or dull areas

Contact marks from the rack, or current density variation

Rack design and part orientation

White bloom after shipping

Residual salts from inadequate rinsing, activated by humidity in transit

Rinse stages and drying before packing

Colour drift between lots

Bath chemistry drift, especially in gold and bronze tones

Bath analysis schedule and colour control on a physical standard


What to write in the specification

1.      Salt spray hours and the failure definition〞 the duration, the standard, and the corrosion area threshold that counts as failure.

2.      Nickel thicknessas a minimum, not a range, plus the decorative layer.

3.      Nickel release requirement with the test standards named, and the parts list it covers, including screws and core wires.

4.      Adhesion test〞 cross-hatch or bend test, so peeling is caught before shipment rather than after.

5.      Colour standard〞 a physical approved sample plus a measured value, because photographs do not control colour.

6.      Report per lot〞 salt spray and nickel release reports tied to the production lot, not to a generic material certificate.

A metal frame is sold on its finish and returned on its finish. The specification above costs one page and replaces the most common after-sales conversation in the category.

Frequently asked questions

Is 48 hours of salt spray enough?

For mainstream retail in temperate markets, it is the usual baseline and a reasonable one. For humid climates, long warranties or premium positioning, specify 72 to 96 hours and confirm the nickel layer thickness that makes it achievable.

Does PVD plating pass nickel release?

PVD itself contains no nickel, so it helps, but the result depends on the substrate and on every metal part that touches the skin. Test the finished frame, not the coating in isolation.

Can I claim nickel free on a stainless steel frame?

Stainless steel contains nickel. The claim needs release test evidence, and in some markets the word "free" is restricted regardless of the measured result. Describe the measured release rather than the material.

Why does the same colour look different between two suppliers?

Because the colour comes from the top layer, and its thickness and chemistry differ. A 0.1 micrometre chromium layer and a 0.3 micrometre one reflect differently, and gold tones shift visibly with a few tenths of a micrometre.

Should hinges be plated to the same specification as the front?

Yes, if they are visible and touch the skin. Hinges and screws are the parts most often left out of the specification and most often responsible for a nickel failure.